Perlite is a glassy volcanic rock with a pearl-like luster. It
usually exhibits numerous concentric cracks that cause it to
resemble an onion skin. A typical perlite sample is composed of 71
to 75 percent silicon dioxide, 12.5 to 18.0 percent alumina, 4 to 5
percent potassium oxide, 1 to
4 percent sodium and calcium oxides, and trace amounts of metal
oxides.
Crude perlite ore is mined, crushed, dried in a rotary dryer,
ground, screened, and shipped to expansion plants. Horizontal
rotary or vertical stationary expansion furnaces are used to expand
the processed perlite ore.
The normal size of crude perlite expanded for use in plaster
aggregates ranges from plus 250 micrometers (µm) (60 mesh) to minus
1.4 millimeters (mm) (12 mesh). Crude perlite expanded for use as a
concrete aggregate ranges from 1 mm (plus 16 mesh) to 0.2 mm (plus
100 mesh).
Ninety percent of the crude perlite ore expanded for horticultural
uses is greater than 841 µm (20 mesh). Crude perlite is mined using
open-pit methods and then is moved to the plant site where it is
stockpiled. Figure 11.30-1 is a flow diagram of crude ore
processing. The first processing step is to reduce the diameter of
the ore to approximately 1.6 centimeters (cm) (0.6 inch [in.]) in a
primary jaw crusher. The crude ore is then passed through a rotary
dryer, which reduces the moisture content from between 4 and 10
percent to less than 1 percent.

After drying, secondary grinding takes place in a closed-circuit
system using screens, air classifiers, hammer mills, and rod mills.
Oversized material produced from the secondary circuit is returned
to the primary crusher. Large quantities of fines, produced
throughout the processing stages, are removed by air classification
at designated stages. The desired size processed perlite ore is
stored until it is shipped to an expansion plant.
At the expansion plants, the processed ore is either preheated or
fed directly to the furnace. Preheating the material to
approximately 430EC (800EF) reduces the amount of fines produced in
the expansion process, which increases usable output and controls
the uniformity of product density. In the furnace, the perlite ore
reaches a temperature of 760 to 980EC (1400 to 1800EF), at which
point it begins to soften to a plastic state where the entrapped
combined water is released as steam. This causes the hot perlite
particles to expand 4 to 20 times their original size. A suction
fan draws the expanded particles out of the furnace and transports
them pneumatically to a cyclone classifier system to be collected.
The air-suspended perlite particles are also cooled as they are
transported to the collection equipment. The cyclone classifier
system collects the expanded perlite, removes the excessive fines,
and discharges gases to a baghouse or wet scrubber for air
pollution control.
The grades of expanded perlite produced can also be adjusted by
changing the heating cycle, altering the cutoff points for size
collection, and blending various crude ore sizes. All processed
products are graded for specific uses and are usually stored before
being shipped. Most production
rates are less than 1.8 megagrams per hour (Mg/hr) (2 tons/hr), and
expansion furnace temperatures range from 870 to 980EC (1600 to
1800EF). Natural gas is typically used for fuel, although No. 2
fuel oil and propane are occasionally used. Fuel consumption varies
from 2,800 to 8,960 kilojoules per kilogram (kJ/kg) (2.4 x 10 to
7.7 x 10 British thermal units per ton [Btu/ton]) of product.